Several different types of deposits can form in HVAC water systems, and terms such as scale, fouling, deposit, film, coating, precipitate, and others are sometimes used interchangeably in the industry to describe these materials. However, it is important to use the correct term in describing these phenomena, because the operating procedures and chemical treatments used to help prevent or delay these deposits from forming, and to remove them when necessary, depend on the specific composition of the deposits.
Deposit refers to any material formed on either the internal or external surfaces of components in contact with water.
Fouling describes the condition of a system in which deposits have formed, including microbiological fouling. Microbiological fouling is slime or biofilm that accumulates by incorporating inorganic particulate matter such as calcium carbonate, silica, and corrosion products.
Scale is formed when the oversaturation of dissolved minerals creates deposits from the water onto heat transfer surfaces or pipes. As water evaporates in a cooling tower or steam boiler, the concentration of dissolved solids becomes greater, and the solubility of particular scale-causing mineral salts can be exceeded. When this situation occurs in a cooling- or steam-water system, scale may form on any surface in contact with the water, especially on heat transfer surfaces. The most common scaling minerals are (1) calcium carbonate, (2) calcium phosphate, (3) calcium sulfate, and (4) magnesium silicate, usually in that order. Most salts are more soluble in hot water than in cold water; however, most calcium and magnesium salts, including calcium phosphate, calcium carbonate, and magnesium silicate, are more soluble in cold water. This is called reverse solubility. As recirculating water passes through the cooling system, the water temperature increases. As a result, calcium and magnesium scales may form anywhere in the system, but most likely on heated surfaces such as heat exchangers or surface condensers. Silica forms in areas having the lowest water temperature, such as in the cooling tower fill.
Minerals such as calcium and magnesium are relatively insoluble in water and can form scale deposits when exposed to conditions commonly found in cooling- and boiler-water systems. For instance, a layer of calcium carbonate scale as thin as 0.40 mm can reduce heat exchanger capacity by 15%.
Several key factors influence whether scale forms:
-
Temperature
-
pH
-
Alkalinity
-
Hardness (concentration of scale-forming salts)
-
Total dissolved solids (influence of other dissolved materials, which may or may not be scale-forming)
-
Phosphate-ortho
-
Silicate/silica
As any of these factors changes, so do scaling tendencies. Changes in pH or alkalinity can greatly affect scale formation. For example, as pH or alkalinity increases, calcium carbonate becomes less soluble and deposits on surfaces.
Some materials, such as silica (SiO2), are less soluble at lower alkalinities. When the amount of scale-forming material dissolved in water exceeds its saturation point, scale may result. In addition, other dissolved solids may influence scale-forming tendencies. In general, a higher level of scale-forming dissolved solids results in a greater chance for scale formation.
Calcium Carbonate Formation (Hard Lime Scale)
The progression of calcium carbonate deposition and scale formation is fundamentally a reversal of the process of creating hard water (when carbonic acid in rainwater dissolves limestone). However, this bond is easily undone once water is put to practical use, because the bicarbonate component of hard water is thermally unstable:
Alkalinity breakdown produces carbonate ion and carbon dioxide (easily lost from a system as a gas). The percentage of bicarbonate broken down increases so long as heat continues to be added to water.
The solubility of calcium bicarbonate is more than 10 000 mg/L. The solubility of calcium carbonate at 24°C is roughly 10 mg/L: 4 mg/L calcium ions and 6 mg/L carbonate ions. Basic chemistry dictates that, for aqueous salts of limited solubility, any effort to increase the concentration of one constituent must cause the concentration of the other constituent to fall. Expressed mathematically, when a soluble salt such as calcium carbonate is dissolved in water, multiplying the concentration of each constituent produces a fixed number Ksp (or solubility product or constant).
Hard water typically contains roughly two bicarbonate ions (HCO3–) for every calcium ion (Ca2+). Cooling tower and boiler makeup water supplies frequently hold up to 300 mg/L hardness or more, which may be further concentrated several times by evaporation in a cooling tower or boiler. Calcium and bicarbonate concentrations may easily approach several hundred mg/L each. Bicarbonate alkalinity breakdown can then lead to levels of 100 mg/L or greater of carbonate ions combined with a near equal concentration of calcium ions to form a very highly supersaturated solution of calcium carbonate, in violation of the solubility product limit.
Scale and sludge are not produced instantly when hard water is introduced into a cooling tower or boiler, because calcium carbonate precipitates only very slowly from a supersaturated solution of calcium and carbonate ions. Such supersaturated solutions are termed metastable, in that there is great potential for precipitation to occur, but induction time is required for its initiation, agglomeration, and adhesion to contact surfaces. For example, hotter heat transfer surfaces speed up initiation and promote formation of the densest crystal structure (calcite). Biofilm in cooling water systems can attract calcium and increase pH locally through protein decomposition (ammonization) to form calcium-carbonate-rich mud and sludge, and carbonate-rich deposits can form on cooling tower fill at wet/dry boundaries due to hypersaturation.
Deposition, Scale, and Suspended-Solids Control
HVAC system treatment strategy is dictated by makeup chemical properties and operating constraints. Treatment of cooling towers fed with makeup water of relatively low hardness is usually quite different than that for cooling towers fed with high-hardness makeup water. In some instances, local water resource conservation or discharge regulations may dramatically affect the treatment strategy used. Manufacturers’ water quality specifications also affect water treatment strategy.
Steam and High-Temperature Heating Water:
-
Makeup water conditioning:
-
Ion exchange (softeners and dealkalizers) to remove calcium, magnesium, and alkalinity.
-
Reverse osmosis (RO) to remove almost all dissolved solids including calcium and magnesium.
-
Deionization (DI) to remove all dissolved solids.
-
Deaeration to aid control of dissolved oxygen, carbon dioxide from carbonate species, and steam condensate pH.
-
Internal chemical treatment of boiler water:
-
Various chemical additives such as sodium hydroxide, sodium carbonate, phosphates, dispersive agents, etc. may be added to “soften” boiler water internally via precipitation of hardness and blowdown, but this practice is considered out of date, and makeup water conditioning is favored. Chemical additives are typically used to address low level hardness not removed by makeup conditioning or due to external contamination.
-
Maintain good internal boiler and steam condensate protection against corrosion to control iron deposition on internal boiler surfaces.
Cooling Towers:
-
Makeup water conditioning:
-
Ion exchange (softening) to remove calcium and magnesium.
-
Reverse osmosis (RO) to remove almost all dissolved solids including calcium and magnesium.
-
Filtration to remove turbidity and suspended metals.
-
Add acid to cooling tower water to remove alkalinity and control carbonate ion formation
-
Add scale inhibitors and dispersants to dramatically slow rate of particle nucleation and agglomeration.
To help determine the tendency of water to form or dissolve calcium carbonate scale, several scaling indices have been developed. These indices are only for indicating the degree of saturation of calcium carbonate scale, not scale of other calcium compounds (such as calcium sulfate). These indices are calculated using the pH, alkalinity, calcium hardness, temperature, and total dissolved solids of the water.
Langelier Saturation Index (LSI). This index was developed to calculate the calcium carbonate scale-forming and scale-dissolving tendencies of drinking (potable) water at or near ambient temperatures (Langelier 1936). Using a water’s calcium hardness, total alkalinity, and total dissolved solids measurements, along with the water’s pH and temperature values, the pH of saturation pH(s) is calculated. Subtracting the water’s pH(s) from its actual pH then results in the LSI. If the water’s measured pH (pH [actual]) is greater than its pH(s) (i.e., positive LSI value; oversaturation), the water has a scale-forming tendency. If the water’s pH (actual) is less than its pH(s) (i.e., negative LSI value; undersaturation), the water will have a scale-dissolving tendency. If the water’s pH (actual) equals its pH(s), it is just saturated and the LSI is zero. Because this index was originally designed to predict calcium carbonate scale in potable water, there are serious deficiencies in the accuracy of this index when applied to evaporative cooling water, heating water, or potable hot water.
The temperature component in the LSI calculation is considered appropriate for water that is carried at ambient soil temperatures through buried distribution piping. However, this was later deemed insufficient for process water used for cooling towers and boilers where values tended almost always to be positive, yet indications of deposition of calcium carbonate were absent. Experience shows that the LSI can be used as a trending value in process water systems to indicate changes in stability, rather than an absolute condition.
The LSI is calculated as
where
| pH(s) |
= |
(9.3 + A + B) - (C + D) |
| A |
= |
[log(TDS) - 1] / 10 |
| B |
= |
-13.12 - log[temp °C + 273] + 34.55 |
| C |
= |
log[Ca2+] - 0.4 |
| D |
= |
log[alkalinity] |
Note: All log values are base 10; alkalinity is the total alkalinity measured as mg/L CaCO3; Ca2+ is the calcium measured as mg/L CaCO3; and TDS is total dissolved solids measured in mg/L.
Ryznar Stability Index (RSI). This index is a more accurate formula for predicting calcium carbonate scale (Ryznar 1944). Ryznar altered the LSI by measuring scale thickness in distributed water systems and comparing the calculated LSI with field results. With this information, he revised the LSI equation. With his formula, an RSI value of 6.0 is considered neutral water, with values > 6.0 indicating a tendency to dissolve calcium carbonate, and values < 6.0 a tendency to deposit calcium carbonate. RSI gives more accurate results than LSI in waters with a pH less than 7.8, but still gives an indication of scale formation at higher pH values. Regardless, the RSI was useful for acid feed water treatment programs, which operated at pH < 7.8.
The RSI is calculated as
where pH(s) is calculated as in the LSI.
Practical (Puckorius) Scaling Index (PSI). Puckorius and Brooke (1991) presented a modified version of the RSI that gives a more accurate and consistent indication of the calcium carbonate scaling potential of cooling water. The PSI takes into consideration the effect of the type of total alkalinity of the cooling water on the measured pH(actual). The measured pH does not always relate correctly to bicarbonate alkalinity, because of the buffering effect of other ions. Rather than using the measured pH in calculating the PSI, an adjusted, or equilibrium pH pH(eq) is used. As with the RSI, a PSI value of 6 indicates a calcium-carbonate-balanced water, and a value lower than 6 indicates a scale-forming tendency. Without scale control treatment, a cooling tower with a PSI of 6 to 7 should operate scale free. Use of the PSI is most applicable when cooling-water pH is above 7.5.
The PSI is calculated as
where pH(s) is as calculated in the LSI, and pH(eq) = 1.465 × log[alkalinity as CaCO3] + 4.54.
Simple models and calculators and more information on these indices can be found online from various sources.
Scale and Deposit Formation Control
Methods used to control scale and deposit formation include the following:
-
Limit the concentration of scale-forming minerals, impurities, and contaminants in a steam boiler or evaporative cooling-water system by intentionally diluting system water from the system via blowdown (bleed-off). This, in effect, lowers concentration that tends to increase during the continuing evaporation of steam or cooling water from these systems. Scale control is thus achieved through operation of the system at subsaturated conditions.
-
Remove scale-forming minerals, impurities, and contaminants before they enter the boiler or cooling-water system, using external or pretreatment systems. This can be done using (1) softened water, blending soft or RO water with other makeup water to achieve a desired saturation index, (2) cycles of concentration, or (3) both methods.
-
Make mechanical changes in the system, such as increasing water flow or surface areas of heat exchangers, to reduce tendencies and potential for scale/deposit formation.
-
Feed acid to reduce alkalinity and keep common scale-forming minerals such as calcium carbonate in solution.
-
Implement a water treatment chemical program designed to control scale and deposit formations in the boiler or cooling-water system.
Retention Time. Controlling cycles of concentration also controls the time that minerals, as well as treatment chemicals and other water constituents, are held within a system. Evaporative-cooling-water systems have a load and volume dependent water residence or turnover time referred to as the holding time index (HTI), also called the half-life retention time of system treatment chemicals, particularly biocides. HTI is the measure of time that it takes for an analyte in the cooling-water system to decrease to 50% of its original value through the process of system losses (blowdown and drift) plus the addition of makeup water to the system. The greater the HTI of the system, the longer water is held in the system and the greater the probability that dissolved, scale-forming minerals will nucleate to produce deposits. At the same time, the greater the HTI of the system, the higher the demand of scale inhibitor, the longer a biocide dosage is held in the system water for a greater contact time to promote microbial kill or control.
HTI for a cooling-water system is calculated as follows:
where
| V |
= |
volume of system |
| BD |
= |
blowdown rate for the system ≈ evaporation rate (ER)/[cycles of concentration (CC) – 1] |
Mechanisms. Water treatment chemical scale inhibitors work by the following mechanisms:
-
Threshold inhibition chemicals control scale formation by dramatically extending the induction time required for deposit to form. If induction time is extended beyond a system’s HTI, mineral deposits fail to form. The most commonly used threshold scale inhibitors are organophosphorus compounds (phosphonates) and low-molecular-weight acrylate polymers. Both classes of materials function as threshold inhibitors; however, the polymeric materials are more effective as dispersants.
-
Scale conditioners modify the crystal structure of scale-forming minerals to render scale nonadherent, fluid, transportable sludge instead of a hard deposit. Scale conditioners include lignin, tannins, and polymeric compounds.
Suspended Solids and Deposition Control
Strainers, filters, and separators may be used to reduce suspended solids to an acceptable level if required. A clean system is more efficient, with less corrosion, scaling, and fouling. Additionally, water treatment is also more effective in a clean system. Therefore, some systems can benefit from using the filtration methods described here.
Strainers. A strainer is a closed vessel with a cleanable screen designed to be removed for cleaning and to retain foreign particles down to 0.025 μm diameter from fluids. Screens with smaller than 0.025 mm (500 mesh) usually create excessive pressure drop for inline pumping. Often, a finer-mesh strainer is used to “clean up” a system after construction and then is replaced with a larger-mesh strainer to reduce pressure drop and the need to clean the strainer as often.
Strainers extract material to protect equipment downstream from constrictions or damage, and to allow saving the extracted product if it is valuable. Strainers are available as manual or automatic cleaning units, and may be made of cast iron, bronze, stainless steel, copper-nickel alloys, or plastic. Supplemental magnetic inserts are available where microscopic iron or steel particles are present in the fluid.
Cartridge Filters. These are typically used as final or tertiary filters to remove nearly all suspended particles from about 0.102 to 0.00102 mm or smaller. Cartridge filters are typically disposable (i.e., once plugged, they must be replaced). The frequency of replacement, and thus the economic feasibility of their use, depends on the concentration of suspended solids in the fluid, the size of the smallest particles to be removed, and the removal efficiency of the cartridge filter selected.
In general, cartridge filters are for systems where contamination levels are less than 0.01% by mass (<100 mg/L). They are available in many different materials and configurations. Filter media materials include yarns, felts, papers, nonwoven materials, resin-bonded fabric, woven wire cloths, sintered metal, and ceramic structures. The standard configuration is a cylinder with an overall length of approximately 254 mm, an outside diameter of approximately 63.5 to 69.85 mm, and an inside diameter of about 25.4 to 38.1 mm, where the filtered fluid collects in the perforated internal core. Overall lengths from 101.6 to 1016 mm are readily available.
Cartridges made of yarns, resin-bonded, or melt-blown fibers normally have a structure that increases in density near the center. These depth-type filters capture particles throughout the total media thickness. Thin media, such as pleated paper (membrane types), have a narrow pore size distribution design to capture particles at or near the surface of the filter. Surface-type filters can normally handle higher flow rates and provide higher removal efficiency than equivalent depth filters. Cartridge filters are rated according to manufacturers’ guidelines. Surface-type filters have an absolute rating, whereas depth-type filters have a nominal rating that reflects their general classification function. Higher-efficiency, melt-blown depth filters are available with absolute ratings as needed. Beta ratios are used to indicate the ratio of particles entering the filter versus those leaving the filter. A high beta ratio means a more efficient filter.
Bag-Type Filters. These filters are composed of a bag of mesh or felt supported by a removable perforated metal basket, placed in a closed housing with an inlet and outlet. The housing is a tubular pressure vessel with a hinged or clamped cover on top for access to the bag and basket. The inlet can be in the cover, in the side (above the bag), or in the bottom. The side inlet is the simplest type. In any case, the liquid enters the top of the bag. The outlet is located at the bottom of the side (below the bag).
The support basket is usually of 304 stainless steel perforated with 3 mm holes. (Heavy wire mesh baskets also exist.) The baskets can be lined with fine wire mesh and used by themselves as strainers, without adding a filter bag. Some manufacturers offer a second, inner basket (and bag) that fits inside the primary basket. This provides for two-stage filtering: first a coarse filtering stage, then a finer one. The benefits are longer service time and possible elimination of a second housing to accomplish the same function.
Filter bags are made of many materials: cotton, nylon, polypropylene, and polyester, with a range of size ratings from <0.00102 to 0.838 mm. Felted materials are most common because of their depth-filtering quality, which provides high dirt-loading capability, and their fine pores. Mesh bags are generally coarser, but are reusable and, therefore, less costly. The bags have a support ring sewn into their opening; this holds the bag open and seats it on top of the basket rim. They can be configured with lift handles, thermal sealed edges instead of sewn stitches, and glazed (thermal pressed) finish to prevent release of fibers. In operation, the liquid enters the bag from above, flows out through the basket, and exits the housing, cleaned of particulate down to the desired size at the specified removal efficiency. The contaminant is trapped inside the bag, making it easy to remove without spilling any downstream.
Sand Filters. A downflow filter is used to remove suspended solids from a water stream. The degree of suspended solids removal depends on the combinations and grades of the medium being used in the vessel. During the filtration mode, water enters the top of the filter vessel. After passing through a flow impingement plate, it enters the quiescent (calm) freeboard area above the medium.
In multimedia downflow vessels, various grain sizes and types of media are used to filter the water. This design increases the suspended solids holding capacity of the system, which in turn increases the backwashing interval, which conserves water. Multimedia vessels might also be used for low-suspended-solids applications, where chemical additives may be required.
Sand filters for cooling-water systems are usually high rate (13.58 L/[s · m2]), with filter media rated from 0.00051 to 0.0102 mm. Some filter vessels are configured to allow water to enter at an angle to create a vortex-shaped filter bed and enhance removal efficiency. Total filtration rate is determined by either system volume turnovers or percent of circulation flow rate. Filter vessels are usually installed sidestream with a booster pump.
When the vessel has retained enough suspended solids to develop a substantial pressure drop, the unit must be backwashed (either manually or automatically) by reversing the direction of flow. This operation removes the accumulated solids out through the top of the vessel.
Centrifugal-Gravity Separators. In this type of separator, liquids enter the unit tangentially, which sets up a circular cyclone flow path. The liquids are accelerated into the separation chamber. Centrifugal forces toss particles denser than the liquid to the side walls of the separation chamber. Solids drop along the perimeter and into the quiescent collection chamber. A low-solids liquid is then drawn into the separator vessel vortex (low-pressure area) and up through the separator outlet at the top of the vessel. Solids are either purged periodically by a manual or automatic timed purge, or continuously bled from the separator bottom outlet to a solids collection/filter chamber. Advantages of separators include a constant pressure drop even as solids are collected, a negligible water loss in the purge cycle, and no backwash or interruption of service. Disadvantages are that they do not remove particles with lower density than the primary liquid (e.g., cottonwood seeds) or fine particles <40 μm, and require periodic mechanical cleaning/service of the collection chamber.
The Handbook Online version of this chapter features separator animations.
General Notes: In specifying filtration systems, third-party testing by an accredited or independent agency should be specified. The test report documentation should include a description of methods, piping diagrams, performance data, and certification.
Filters described in this section may also be used where industrial process cooling water is involved. When they are installed next to cooling towers, filter piping is used to sweep tower basin floors clean at a rate of 0.68 to 1 L/(s·m2) via sweep ejector nozzles that can draw sediments behind the nozzles. This usually calls for a bigger booster pump to create the sweeping action. For this type of service, consultation with the filtration equipment manufacturer is essential to ensure proper application.
2.2 CORROSION AND CORROSION CONTROL
Corrosion is the destruction of a material, usually a metal or alloy, but it can include nonmetals like plastics, concrete, lumber, etc. The destruction process can be through chemical or electrochemical reaction with its environment. Common examples of those that can react are magnesium, aluminum, zinc, chromium, iron, tin-nickel, and lead. Examples of pure metals that are less reactive include copper, silver, platinum, and gold. Exceptions exist depending on the character of metal oxide surface films. Very tenacious surface oxide films can block corrosion of metals such as aluminum, chromium, nickel, and stainless steels. Corrosion is therefore a two-step process: (1) setting up reactive sites (anodes and cathodes) on contact surfaces and (2) establishing a continuing reaction between water and metal.
Depolarization involves a chemical reaction that fully or partially removes or weakens protective surface oxide films, thereby exposing base metal. Acidic conditions tend to dissolve protective films and produce uniform metal loss. High chloride tends to weaken protective film on metals so that subsequent corrosion is more irregular.
In most instances, the second reaction is electrochemical in nature, much like that in an electric battery. For corrosion to occur, a corrosion cell consisting of an anode, a cathode, an electrolyte, and an electrical connection must exist. Metal ions dissolve into the electrolyte (water) at the anode, leaving behind electrons. These electrons flow through the metal (electric connection) to other points (cathodes) where electron-consuming reactions occur. The result of this activity is the loss of metal from the anode and often the formation of a deposit at the cathode. The rate of corrosion depends on the rate of flow of the electrons. Mechanisms for various types of corrosion are shown in Figure 1.
Types of Corrosion
Corrosion is often categorized into three broad categories: (1) readily identifiable through visual examination, (2) identifiable with supplementary means of examination, and (3) verifiable with microscopy. Group 1 covers the most prevalent types: general corrosion, localized corrosion, and galvanic corrosion for aqueous environments. Localized corrosion covers pitting, crevice corrosion, cracking, galvanic, and under-deposit corrosion. Many other types of corrosion associated with these three main categories are of concern in water treatment and encountered in boiler and cooling water systems for both HVAC and processes, including stress, fatigue, crevice, erosion, and microbiologically influenced corrosion. Corrosion in practical systems is rarely of one type but can be the result of an aggregate of several forms.
Uniform (general) corrosion (Figure 1D) is the most common type and is caused by a chemical or electrochemical reaction that results in the deterioration of the entire exposed surface of a metal.When general attack is due to chemical reactions, it is usually the result of either acid (low pH) or caustic (high pH) attacks. In near chemically neutral environments, general attacks are often initiated with differential oxygen concentrations, compounded with biofilms and deposits that create electrolytic anodes and cathodes on contact surfaces. General corrosion removes and weakens whatever protective metal oxide surface film may be present on a metal. Wetted metal surfaces below 66°C are often coated by biofilm. Beneath biofilm, pH is lower than in bulk phase water due to microbiological metabolism. This lower relative pH tends to weaken protective oxide surface films and expose subsurface elements to corrosive hydrogen ions.
Biological activity in and beneath biofilms also produces enzymes reactive with protective metal oxide surface films. Low pH and high chloride are primary contributors to the removal of protective iron oxide films from steel. Ultimately, metal can deteriorate to the point of failure. Uniform attack corrosion accounts for the greatest amount of metal destruction by corrosion but is considered a normal condition when metals are exposed to water-based fluids, because it is (1) evenly distributed over a given metal surface throughout a system and (2) predictable, manageable, and often preventable. Uniform corrosion can be compensated for by using corrosion-resistant construction materials, applying protective coatings, or providing appropriate cathodic corrosion protection. In some (but not all) cases, uniform corrosion can be controlled by changing the chemical environment. Raising pH and reducing chloride and total dissolved solids can reestablish protective surface oxide films on steel and ferrous alloys. The effects of uniform corrosion can be anticipated through measurement of material specimens exposed to the anticipated operating environment in a corrosion coupon rack. Metallic coupons are inserted in the rack for a predetermined exposure before being removed, cleaned, weighed, and examined to determine rates of corrosion. Corrosion rates can also be measured with electrical probes and ultrasonic pipe wall thickness testers.
Localized (pitting) corrosion (Figure 1E) results from breakdown of surface protective oxides. Breakdown can be due to environmental factors, defective material, or inconsistent surface conditions. When a small defect or hole forms in protective metal oxide surface film, usually as the result of inconsistent inhibitor film formation at that location, this area becomes electrochemically anodic, while part of the remaining metal becomes cathodic, producing a localized galvanic reaction, often referred to as a concentration cell. The deterioration of this small area penetrates the metal and can quickly lead to failure. This form of corrosion is often difficult to detect because it is usually relatively small and may be covered and hidden by corrosion-produced compounds (corrosion byproducts). Pitting is often the most serious form of corrosion, because the action is concentrated in a small area.
Continued corrosion reaction in pits of ferrous metals can cause the appearance of hollow, tube-like growths above the metal surface, called tubercles. These are formed by layering deposits of iron oxide species, a by-product of the pit formation at the base of the tubercle. Like corrosion cells, pits may reach an autocatalytic stage of rapid corrosion, though not always. Tubercles, however, are always the result of an autocatalytic process. Unlike crevice corrosion, pitting is thought to be self-initiated in otherwise unmarred surfaces by the presence of deposits and chloride salts. The pit then concentrates chlorides in the hollow. The process is accelerated by the presence of oxygen and bacteria, which creates a localized adjacent cathode to the anodic surface of the pit, forcing concentrated anodic deterioration and enlarging the pit. See the section on Microbiologically Influenced Corrosion for more information.
Galvanic (dissimilar metal) corrosion (Figures 1A and 2) occurs when two different metals are located together in an electrolyte (solution). A galvanic couple forms between the two metals, where one metal becomes the anode and the other the cathode. The anode, or sacrificial metal, corrodes and deteriorates faster than it would alone, while the cathode deteriorates more slowly than it would otherwise. Galvanic corrosion is limited to the immediate area of the juncture of the two dissimilar metals. Deterioration of the anodic metal is most severe at the point of contact and diminishes markedly with distance. Galvanic corrosion rarely extends more than a few inches from where dissimilar metals make contact.
Three conditions must exist for galvanic corrosion to occur:
-
Electrochemically dissimilar metals must be present.
-
The metals must be in intimate electrical contact.
-
The metals must be exposed to an electrolyte.
Common examples of galvanic corrosion in water systems are metal-to-metal contacts between steel and copper alloys (brass); aluminum and steel; galvanized (zinc) steel and steel or iron; and carbon steel and stainless steel. If galvanic corrosion occurs, the metal named first is the anode and experiences the corrosion.
Stress corrosion cracking (SCC), or environmental cracking, can result from a combination of corrosive environmental conditions affecting the metal and in alloys subject to tensile stress. The stress may be applied, residual (from processing), or a combination. The resulting crack formation can be transgranular or intergranular.
Corrosion fatigue is a result of combined action of cyclic stresses and a corrosive environment. Cyclic stresses (e.g., from rapid heating and cooling) are concentrated at points where surface defects exist, and corrosion has roughened or pitted the metal surface. Corrosive environments promote crack growth and reduce fatigue strength because of the action of applied cyclic stresses where a protective oxidation film fails on metal surfaces.
Caustic cracking occurs when metal is stressed in a fluid with a high caustic content, and a mechanism of concentration occurs at high water temperature in presence of silica. It is also known as caustic embrittlement. It occurs in boilers due to overfeeding, resulting in increasing caustic concentrations.
Crevice corrosion (Figure 1B) occurs in the void between a metal and another surface. These opposing surfaces can be metal (similar or dissimilar), gaskets, organic residue, or scale deposits. In this void, and usually in the presence of a stagnant solution, a localized corrosion environment is created. Also referred to as under-deposit corrosion, it is like concentration cell corrosion issues. As in pitting, the crevice allows the concentration of chlorides in the void and depletion of inhibitors and of oxygen, causing the crevice to become anodic and acidic to accelerate the reaction.
Erosion corrosion (flow-accelerated corrosion) occurs because of flow or impact that can physically remove inhibitor films and the protective metal oxide surface. This type of corrosion usually occurs because of altered flow patterns or a flow rate that is above design. Suspended solids in a solution can greatly contribute to erosion corrosion. Control of suspended solids, reduction of turbulence, and avoiding use of soft metals can reduce erosion in systems and enhance material life cycle and durability.
Cavitation corrosion, a form of erosion corrosion, is caused by the rapid formation and collapse of vapor bubbles during a change in fluid pressures to below its vapor point in a solution and adjacent to a metal surface.
Microbiologically influenced corrosion (MIC), also called microbial corrosion, bacterial corrosion, or biocorrosion, involves the reaction of microbiological species with metals. It is caused or promoted by microorganisms, usually chemoautotrophs, which are microbes (usually bacteria) that can produce corrosive acids and enzymes as a part of their cellular metabolism. Bacteria do not attack metal or protective metal oxide surface films. Bacteria influence the chemical reactions between cathodic and anodic areas. The acids and enzymes cause attack, especially when bacteria create a biofilm. MIC can be a very serious problem in building HVAC recirculating water systems and wet sprinkler systems, involving many forms, mechanisms, and types of microbiological organisms, including the following.
-
Iron-related bacteria (IRB), such as Gallionellea ferrugine, Leptothrix ochracea, Cranothrix polysporer, and Ferrobacillus species, cause corrosion of iron and steel in recirculating water systems by direct metabolism of iron. Some of these organisms consume iron as a part of their metabolic process and then deposit it in the form of hydrated ferric hydroxide along with mucous secretions. Iron bacteria are commonly found in all types of cooling systems, especially in low-flow areas.
-
Sulfate-reducing bacteria (SRB) are the best known group of organisms involved in MIC. These anaerobic organisms (i.e., they live without metabolizing oxygen) metabolize sulfur in one form or another. The most widely known, Desulfovibrio, is often found in cooling systems, especially where oil or sludge is present. Metabolic processes involve the transfer of electrons from a “food source” to an electron acceptor (oxidizing agent) for the purpose of obtaining energy and the building blocks for continued cell growth. The principal electron acceptor under aerobic (oxygen rich) conditions is oxygen. When oxygen is depleted or absent, SRBs can use sulfate as an alternative electron acceptor to oxygen. In the process, sulfate is converted to corrosive hydrogen sulfide.
-
Acid-producing bacteria (APB) include the slime-forming bacteria Pseudomonas, Aerobacter, and Bacillus, which exude compounds such as formic, acetic, and oxalic acids in their metabolic processes. These organic acids cause low-pH conditions at local sites, resulting in corrosion. Thiobacillus is a common APB that oxidizes sulfur compounds into sulfuric acid, which is extremely corrosive and leads to localized under-deposit and pitting corrosion, often resulting in pinholes in system piping.
-
Biological deposits (BD; also called biofilms) such as algae, yeast, molds, fungi, and bacterial slimes can also cause MIC. Even in the absence of specific corrosive organisms, biological deposits establish an environment for corrosion by establishment of concentration cells and lowering pH, resulting in under-deposit corrosion. Biological deposits also act as traps providing food for other organisms, accelerating metabolism and growth. This complex matrix sets up a corrosion potential between adjacent areas of a metal surface that may have different types of deposits. In general, the longer biological deposits are allowed to flourish, the more difficult, time consuming, and expensive they are to bring under control. They also create high resistance to flow (friction factor) and reduce heat transfer.
To control and/or prevent MIC, it is important to understand the processes that cause it. An effective control and prevention program must address all types of biological growths in recirculating water systems.
Factors Affecting Corrosion
All cooling-water system metals of construction will corrode at some rate. Therefore, the rate of corrosion is of prime importance. This rate is commonly expressed in terms of penetration (thickness of metal lost) as millimetres. Table 2 provide guidelines for categorizing corrosion rates.
The following paragraphs describe the effects of various factors on corrosion.
Moisture. Corrosion does not occur in dry environments. However, some moisture is present as water vapor in most environments. In pure oxygen, almost no iron corrosion occurs at relative humidity up to 99%. However, when contaminants such as sulfur dioxide or solid particles of charcoal are present, corrosion can proceed at relative humidity of 50% or more. The corrosion reaction proceeds on surfaces of exposed metals such as iron and unalloyed steel as long as the metal remains wet. Many alloys develop protective corrosion-product films or oxide coatings and are thus unaffected by moisture.
Oxygen. Oxygen dissolved in water (DO) is a depolarizer at cathodes of corrosions cells, sets up differential aeration cells on metal surfaces, and feed aerobic bacteria to support MIC. However, it does not lead to continuous corrosion of active metals such as aluminum, chromium, nickel, and zinc because these metals form protective oxide surface films with dissolved oxygen acting as polarizing barriers that separate potentially oxygen-reactive metal from DO. Basic ferrous metals (steel and iron) form only porous oxide films susceptible to depolarization by numerous chemical and mechanical influences. Once depolarization of surface film on steel occurs, DO perpetuates the attack at anodes unless a protective film is formed and maintained by corrosion inhibitors (which reestablish film integrity). DO is needed for molybdate, a commonly used corrosion inhibitor, to work effectively.
pH. The pH of cooling water influences the potential of most metals to corrode. Corrosion tends to increase as pH levels decrease (become more acidic) because protective surface film tends to weaken or dissolve as pH falls below 7.0. However, different metals show different corrosion curves with respect to pH. Basic solutions are generally less corrosive to ferrous systems because they tend to make surface oxide film less soluble. It is practical in many water systems to minimize corrosion by adding caustic or alkaline buffering agents to raise and stabilize the pH between 9 and 11. Aluminum corrodes in both low pH (<4) and above a pH of 8.5 because its protective film weakens or dissolves outside this range; this reduces the acceptable range of pH in systems that contain both steel and aluminum.
Chlorides. Chloride is nonvolatile, commonly found in water, easily concentrated as water evaporates. Chloride ions can be adsorbed with the metals’ protective surface film, weakening the film and making metal progressively more vulnerable to pitting and general corrosion, as chloride concentration rises and/or pH falls. Once protective film is depolarized, exposed elemental metal (generally ferrous and copper alloys) is free to react with oxygen. Because depolarization establishes an electrochemical circuit, the rate of reaction depends not only on the amount of oxygen present but also on the electrical conductance of the water; the higher the chloride and all other ionic species such as sulfate, sodium, potassium, etc., the more readily electrochemical activity proceeds.
Increasing the concentration of dissolved solids increases the conductivity of the electrolyte (water). Because a corrosion cell depends on the ability of the electrolyte to conduct the flow of electrons, the presence of more dissolved solids increases corrosion. For the corrosion reaction to proceed, a potential difference between anodic and cathodic areas is required. The potential difference between locations on a metal surface is caused by variations in solute concentration in the localized environment. The increase in corrosion caused by such conditions is called concentration cell corrosion. Crevices, cracks, pits, and foreign deposits on the metal surface can create conditions that contribute to corrosion due to differential dissolved oxygen levels. The anodic area, where corrosion proceeds, is in the crevice or pit, or under the deposit. Whether the process is metal ion or oxygen concentration based, available chlorides accelerate the reactions. The process turns into an autocatalytic reaction, resulting in rapid destruction of the metal alloy. Though slow to start, once chlorides are introduced, this series of events leads to rapid failure of the metal unless replaced with corrosion-resistant material, isolated by an impervious coating, or properly inhibited.
Galvanic (Dissimilar Metal) Corrosion. Another factor that accelerates corrosion is the difference in potential of dissimilar metals coupled together and immersed in an electrolyte. The following factors control the severity of corrosion resulting from such dissimilar metal coupling:
-
Relative differences in position (potential) in the galvanic series, with reference to a standard electrode (see Figure 2): the greater the difference, the greater the driving force of the reaction.
-
Relative area relationship between anode and cathode: because the amount of current flow (and therefore total metal loss) is determined by the potential difference and resistance of the circuits, a small anodic area corrodes more rapidly in the presence of a large cathodic area. A larger anodic area relative to the cathode reduces the corrosion rate.
-
Intentional polarization of either cathodic or anodic areas: technology is available to create polarization to reduce the potential difference between components of piping systems, large storage tanks, and various metal structures and thus reduce the rate of attack at points of naturally occurring anodic activity.
-
Ionic content of water or electrolyte: as the concentration of the ionic components of the electrolyte increases, the resulting higher electrical conductivity increases the rate of galvanic corrosion because the resistance to electron flow through water is reduced. Metal ions that are of higher galvanic potential than the contact metal may plate out on the contact metal surface and cause local galvanic corrosion.
Stress. Stresses in metallic structures rarely have significant effects on the uniform corrosion resistance of metals and alloys. Stress may be due to mechanical loading, vibration, large or cyclic temperature swings, repeated impact, or chemical or MIC gouging (acting alone or in combination). Stresses in some metals and alloys can cause corrosion cracking when the metals are exposed to specific corrosive environments. The cracking can have catastrophic effects. Almost all metals and alloys exhibit susceptibility to stress corrosion cracking in at least one environment. Common examples are steels in hot caustic solutions, high-zinc-content brasses in ammonia, and stainless steels in hot chlorides. Metal manufacturers have technical details on specific materials and their resistance to stress corrosion.
Temperature. Higher temperatures speed up chemical reactions and weaken protective surface films. Thus, corrosion rates are greatest in areas where temperatures are the hottest. Even temperature variations within a single piece of metal cause the warmer areas to become anodic to the cooler areas and corrode.
An increase in temperature may increase the corrosion rate, but only to a point. Oxygen solubility decreases as temperature increases and, in an open system, may approach zero as water boils. Beyond a critical temperature level, the corrosion rate may decrease because of a decrease in oxygen solubility. However, in a closed system, where oxygen cannot escape, the corrosion rate may continue to increase with an increase in temperature until the oxygen is used up. For those alloys that depend on oxygen in the environment for maintaining a protective oxide film (e.g., stainless steel), the reduction in oxygen content caused by an increase in temperature can accelerate the corrosion rate by preventing oxide film formation.
Temperature can affect corrosion potential by causing a salt dissolved in the environment to precipitate on the metal surface as a protective layer of scale. One example is calcium carbonate scale in hard waters. Temperature can also affect the nature of the corrosion product, which may be relatively stable and protective in certain temperature ranges and unstable and nonprotective in others. For example, zinc sacrificial anodes are ineffective in systems over 65.6°C.
Pressure. Where dissolved gases such as oxygen and carbon dioxide affect the corrosion rate, pressure on the system may increase their solubility and thus increase corrosion. Similarly, a vacuum on the system reduces the solubility of the dissolved gas, thus reducing corrosion. In a heated system, pressure may rise with temperature. It is impractical to control system corrosion by pressure control alone.
Flow Velocity. The impact of flow velocity on corrosion rate depends on several factors, including
-
Amount of oxygen in the water
-
General chemical environment (e.g., low pH, high chlorides, high MIC potential due to sulfates)
-
Temperature
-
Suspended solids in the water
-
Type of metal exposed (copper and iron are both susceptible)
-
Flow rate
In metal systems where corrosion end products retard corrosion by acting as a physical barrier, high flow velocities may erode these protective barriers and increase the potential for corrosion. An excessively turbulent environment may cause uneven impingement attacks, from both erosion and corrosion. As mentioned earlier, this is called erosion corrosion. It is commonly found in piping with sharp bends and inlet ends of small openings where the flow velocity is high. Copper and softer metals are more susceptible to this type of attack. When flow velocity is low (less than 1 m/s), suspended solids can drop out and cause deposition as well as under-deposit corrosion, including concentration cell corrosion and microbial corrosion. Low flow velocity can also affect transport of corrosion inhibitors and polarization of corrosion cells.
Insoluble Solids (Turbidity) Management. The presence of solids, either suspended or deposited, in the waters of HVAC and process systems can cause abrasion, enhance corrosion, and reduce heat transfer. Suspended solids in flowing waters increase erosion corrosion and biofouling. Under-deposit corrosion can form under dust, dirt, rust, silt, and other solids introduced into evaporative cooling-water systems; mud, rust, and silts can deposit in closed-loop piping systems, especially in dead legs, storage and heat exchanger tanks, end bells, or cast iron boiler sections. See the section on Deposition, Scale, and Suspended-Solids Control for further discussion of control.
Other major factors affecting corrosion include those discussed in the microbiological and fouling control sections. They center on the contaminants and/or conditions that work to
-
Prevent inhibitors from reaching the metal surface
-
Remove inhibitors and/or protective films from the metal surface
-
Promote the formation of biofilm and/or deposits under which corrosion can occur
Such conditions can be common in systems with high suspended matter and/or poor microbiological control programs, as well as those systems with process contamination and/or poor deposit control programs, including poor corrosion control programs contributing corrosion debris (byproducts) as deposits. This highlights the importance of system maintenance and a good water treatment program to ensure system efficiency and longevity.
Corrosion Preventive and Protective Measures
Materials Selection. Any piece of heating or air-conditioning equipment can be made of metals that are virtually corrosionproof under normal and typical operating conditions. The specific choice of materials used in a system or piece of equipment must consider the expected operating conditions, potential upset conditions, expected system, lifetime, ease of replacement, and of course budget. The availability of many materials of construction options helps ensure that the proper choices can be made for a successful service life in most cases. When selecting construction materials, the following factors should be considered:
-
Corrosion resistance of the material in the operating environment, including water quality.
-
Corrosion products that may be formed and their effects on equipment operation.
-
Ease of construction using a particular material.
-
Design and fabrication limitations on corrosion potential.
-
Economics of construction, operation, and maintenance during the projected life of the equipment. Expenses may be minimized in the long run by paying more for a corrosion-resistant material and avoiding regular maintenance.
-
Use of dissimilar metals should be avoided. Where dissimilar materials must be used, insulating gaskets and/or applied coatings must be used to prevent galvanic corrosion.
-
Compatibility of chemical additives with materials in the system.
-
Building codes and regulations.
Protective Coatings. The operating environment has a significant role in the selection of protective coatings. The suitability of a coating for a particular environment also depends on the surface preparation of the metal to be protected, coating thickness, and coating application technique. Coating durability depends on the adhesion between the coating and the metal. Adhesion depends greatly on surface preparation, including cleaning, degreasing, and the application of primers.
Defects in a coating are difficult to prevent. These defects can be flaws introduced into the coating during application or mechanical damage sustained after application. To maintain corrosion protection, defects must be repaired both in the fabrication process and in the operational environment. Defects in coatings, called holidays, can lead to significant localized corrosion of the base metal, most commonly in the form of oxide lifting or cathodic disbondment. Oxide lifting occurs when anodic corrosion products accumulate under a coating adjacent to holidays, lifting the coating from the protected surface. Cathodic disbondment is the result of the cathodic reduction of dissolved oxygen, which, along with water, migrates under the coating from holidays. Once under the coating, blistering occurs, separating the coating from the protected surface.
Cycles of Concentration. Improved corrosion control may be achieved by optimizing the cycles of concentration (the degree to which soluble mineral solids in the makeup water have increased in the circulating water because of evaporation). Generally, adjustment of the blowdown rate and pH to produce a slightly scale-forming condition (see the section on Scale and Deposit Formation Control) results in an optimum condition between corrosion and scale formation.
Chemical Methods. Historically, several chemicals have been used to inhibit corrosion and scale formation. It is important that the inhibitors do not interfere with the heat transfer or other functions of the metal. In general, corrosion inhibitors function in one of three ways:
-
Passivation: these inhibitors form a thin protective oxide film on the metal surface, usually at anodic sites. Nitrites and molybdates work in this way.
-
Precipitation: these inhibitors contain materials that are precipitated out of solution to form protective films at both cathodic and anodic sites in a corrosion cell. Silicates and phosphates work this way. They require oxygen for effective inhibition.
-
Adsorption: these inhibitors are directly adsorbed onto the metal surface, where they form a protective layer. Organics usually function in this manner.
Many inhibitors work best when initially applied at two to three times their normal dosage for several weeks. This pretreatment procedure improves corrosion control by rapidly establishing the protective inhibitor films to new metal surfaces. This procedure should also be repeated for start-ups that follow shutdowns and any time pH or other deviations occur.
Film-forming chemical inhibitors reduce or stop corrosion by interfering with the corrosion mechanism. Inhibitors usually affect either the anode or the cathode. The most common inhibitors are molybdates, phosphates, zinc, phosphonates, silicates, nitrite-borates, aromatic azoles, and organics. Although very effective, chromate inhibitors are severely restricted because of their environmental toxicity and federal laws that have banned their use. The most important factor in an effective corrosion inhibition program is consistent control of both the corrosion inhibition chemicals and the key water characteristics. No program will be effective without controlling these factors.
Anodic corrosion inhibitors establish a protective film at the anode. They stop the corrosion cell by blocking the electrochemical reaction at anodic sites and reestablishing polarization. Though these inhibitors can be very effective, they can also be very dangerous if insufficient anodic inhibitor is present, because the entire corrosion potential can be focused at unprotected anode sites. Severe localized pitting attack can occur at unprotected anodic sites if insufficient inhibitor is present.
Cathodic corrosion inhibitors retard oxygen reduction at the cathode, form protective films at cathodes, and slow overall electrochemical activity. Cathodic inhibitors are not as effective as fully deployed anodic inhibitors, but are commonly used in conjunction with anodic inhibitors to reduce anodic inhibitor dosage requirement.
Combination corrosion inhibitors protect by forming a film on all metal surfaces, whether anodic or cathodic. Optimum corrosion inhibition is typically obtained through use of one or more anodic and/or cathodic inhibitor(s).
Adsorptive filming inhibitors are hydrophobic chemical additives that form a molecular film on metals to create a barrier to corrosion (analogous to paint but much thinner). A filming inhibitor bonds to metal through direct molecular charge interaction between the inhibitor and the metal’s surface due to opposite electrical charge. Such bonding is quite strong. The class of copper corrosion inhibitors termed azoles is a good example.
Cathodic Protection. Sacrificial anodes reduce galvanic attack by providing a metal (such as zinc or magnesium) that is more active (anodic) in the galvanic series than two metals in a galvanic couple. A sacrificial anode becomes anodic to the surface metal and supplies electrons to relatively cathodic surfaces, thereby limiting the corrosion of the more anodic metal in the galvanic couple. Proper design and placement of anodes is important. When properly used, they can reduce loss of steel from the tube sheet and head cover of heat exchangers. Sacrificial anodes have helped supplement chemical programs in many cooling-water and process water systems.
Impressed-current protection is a similar corrosion control technique that reverses the corrosion cell’s normal current flow by impressing a stronger current of opposite polarity. Direct current is applied to an anode (inert [platinum, graphite] or expendable [aluminum, cast iron]), reversing the galvanic flow and converting the steel from a corroding anode to a protective cathode. The method is very effective in protecting essential equipment such as elevated water storage tanks, steel tanks, or buried pipelines and structures.
Uniform, or general, corrosion can be quantitatively measured. Localized corrosion, by definition, may only be observed in some cases, and is unobservable in most cases. Although the process of localized corrosion itself is not measurable, damage to metals by localized corrosion attack can be assessed through various means, such as eddy current testing of chiller tubes.
Corrosion Coupons. Using corrosion coupons is an accepted method for evaluating uniform corrosion rates in both closed- and open-loop systems. Coupon specimens can sometimes exhibit results of localized attack, most frequently from under-deposit and/or microbiologically influenced corrosion. Evidence of excessive localized attack on a coupon specimen may indicate invalid installation of the coupon specimen due to inadequate flow velocity and wrong position against the direction of flow. Careful selection, handling, placement, alignment, and recording of coupon specimens is required for accurate test results. Corrosion coupon racks are designed to comply with ASTM Standard D2688 to provide indication of adequate flow and direction of flow. Adequate flow rates and velocities of the fluid through the coupon rack are also essential to reflect system operating conditions: velocity of 1 m/s is normally used, and velocities in excess of 1.5 m/s may influence erosion, particularly of soft metals such as copper. Ideally, constant flow should be maintained throughout the test period and variable-flow piping systems should use pressure-independent flow control devices (automatic flow regulators) in the coupon rack piping. Coupon specimens should not be disturbed during a test.
Mild steel and copper are commonly used as coupons; admiralty grades of brass and various grades of stainless steel are less common. Regardless, coupon selection should reflect system metallurgy. Placement of the least noble coupon specimen should precede progressively more noble coupons in the rack in the direction of fluid flow.
Because of high initial corrosion rates of the specimen coupon metals, long-duration tests of coupons (60 to 90 days) yield more accurate results in operating systems than shorter tests (15 to 30 days). For new systems, first-30-days tests can indicate the level of passivation during startup. For comparison and trend analysis, a series of tests should be conducted using the same or similar exposure lengths.
Electronic corrosion sensors or probes can be used to determine uniform corrosion rates in a system or to augment a corrosion coupon program. Many different types of probes and systems are available, including electric resistance, linear polarization resistance, electrical impedance microscopy, and acoustic wave emission probes. Linear polarization resistance and electrical resistance are common methods to give real-time feedback of corrosion rates. However, because rates of uniform corrosion are rarely consistent over time, the readings from linear polarization devices should be monitored or data-logged to assess trends in corrosion rates and system stability. Electronic sensors do not exhibit the clear differences between uniform and localized attack that may be observable on coupon specimens. Consult a water treatment professional about the proper type of probe for the specific application and water treatment program.
2.3 BIOLOGICAL GROWTH CONTROL
Most heating equipment operates above normal biological temperature limits and therefore has fewer microbial problems. Hydronic systems operated below about 50°C provide conditions for growth and proliferation of microorganisms: abundant water, aeration, a possible supply of nutrients, and surfaces upon which to attach. Nutrients may include inorganic and organic compounds added directly to fight corrosion/scale/foam (e.g. nitrites, phosphate, phosphonate) or introduced as a process or operational contaminant. Problems associated with the uncontrolled growth of microorganisms in cooling or low-temperature heating water systems can be categorized in the following four areas:
-
Plugging and fouling by biological slime (biofilm/biomass)
-
High energy consumption due to biofilm presence
-
Biodeterioration (e.g., wood rot)
-
Microbiologically influenced/induced corrosion (MIC)
-
Potential health/safety issues (e.g., disease-causing bacteria)
Microbiological activity depends on, and reacts to, the specific conditions of a given water system. Clean, municipally treated, drinking (potable) water likely has extremely low biological activity. Wastewater and sewage are most likely highly biologically active. There are a vast number of different biological entities that can potentially be found in water, and the topic of microbiology is far too complex for involved discussion in this context, but there are a few key microbiological concepts that are very important to water treatment:
-
All practical water systems have some degree of biological activity.
-
Assimilable carbon is the primary component of biological activity, along with nitrogen and phosphorous.
-
Biological activity appears in two forms: freely circulating organisms (planktonic) and organisms attached to surfaces (sessile); the same organism types may be found circulating or in biofilms.
-
Sessile organisms form biofilm, which is present in all water conduits to a degree (even human arteries and the human digestive tract).
-
Metabolism is an oxidation/reduction process involving transfer of electrons from an electron source (food/nutrient) to an electron acceptor, most commonly oxygen. Through this process, organisms obtain energy and the building blocks for growth and reproduction.
-
Metabolism is fostered by biological catalysts (enzymes).
-
Metabolism produces inorganic and organic waste products, which tend to be acidic/corrosive.
-
Some organisms (aerobic) require oxygen to maintain metabolism and die or go dormant in the absence of oxygen (obligate aerobes).
-
Some organisms (anaerobic) only use other electron acceptors (oxidizing agents), such as sulfate, and die or go dormant in the presence of oxygen (obligate anaerobes).
-
Some organisms can metabolize with or without oxygen (facultative anaerobes).
-
Chemical/biochemical conditions (e.g., pH, oxygen level, enzyme presence) may be considerably different under biofilm than in general water circulation (bulk phase water).
-
Biofilm mass depends on nutrient availability, flow velocity, temperature, and oxygen.
-
Small particles of biofilm, containing many microbes, freely detach from biofilm to migrate within a system and promote biofilm extension
Microorganisms found in cooling-water systems generally fall into one of four categories: (1) bacteria, (2) algae, (3) fungi, or (4) macro higher forms. These organisms can enter a cooling system in various ways: through the makeup water supply; from the atmosphere during normal operation; or from accumulations of environmental organic matter such as insects, bird droppings, grass clippings, and construction debris. Microbial growth can interfere with a cooling operation by causing fouling or corrosion and may pose a health hazard.
Bacteria. When considering biological growth in a cooling system, it is important to distinguish between planktonic (free-living) and sessile (attached) microorganisms:
-
Planktonic bacteria are suspended in the water and sometimes referred to as “free floaters” or “swimmers.” These are aerobic bacteria that thrive in an oxygenated environment. They are not harmful to the cooling system, because they do not directly cause deposits or corrosion, but they can provide nutrients for other microorganisms. Usually, the count of planktonic bacteria increases with increasing organic carbon nutrient as measured by the water’s chemical oxygen demand (COD) or its total organic carbon (TOC) content. In addition, some planktonic bacteria, such as Legionella pneumophila, are pathogenic and can present a significant human health risk.
-
Sessile bacteria are non-swimming (attached) bacteria, sometimes called “stickers.” Sessile organisms cause most corrosion problems in cooling-water systems, because they are not detected in total bacteria counts and tend to be overlooked until problems arise. They establish themselves by attaching to contact surfaces to develop microcolonies with dense biomatrix structures. Sessile bacteria types include slime formers and anaerobic (corrosive) bacteria. Slime formers can grow and form gelatinous deposits on almost any surface in contact with the cooling water. These deposits are viscoelastic and can grow so large that they restrict water flow and interfere with heat transfer. They also may promote under-deposit corrosion. Usually, if slime formers are present in the system, deposits can be felt on the sides of the cooling tower basin just below the water level. Anaerobic bacteria thrive in oxygen-deprived environments and often establish colonies beneath slime deposits or under other types of deposits. Surface microbial measurements using special mesh coupons and/or other monitoring devices can be used to monitor sessile bacteria.
Biological fouling can be caused by a wide variety of organisms that produce biofilm and slime masses. Slimes can be formed by bacteria, algae, yeasts, or molds and frequently consist of a mixture of these organisms combined with organic and inorganic debris. Sulfate-reducing bacteria (SRB), slime-forming bacteria (SFB), and iron-related bacteria (IRB) are the most concerning species (after Legionella). Their presence suggests a potential for severe corrosion and fouling. IRB are commonly found in tubercles and assimilate ferrous ions to form mounds of ferric hydroxide, whereas SRB are usually found in the bottom of tubercles with black iron sulfides and sometimes elemental sulfur. The sulfur products give off a rotten egg smell. They signal the presence of acid-producing bacteria and deep penetrating pits.
Because biofilm microorganisms can dramatically enhance, accelerate, and, in some cases, initiate localized corrosion (pitting), they are tested and monitored in critical heat transfer operations. Monitoring methods include the following:
-
Visual and tactile inspection
-
Water analysis for ammonia, chemical oxygen demand (COD), total organic carbon (TOC), adenosine triphosphate (ATP), bacteria speciation’s, and planktonic plate counts
-
Online biofilm monitors, including corrosion-resistant coupons, disks/plugs, electrochemical sensors, fluorometry, thermal gradient sensors, and sidestream devices to track hydrodynamic pressure differential and heat transfer
Microorganisms can influence localized corrosion directly by their metabolism or indirectly by the deposits they form. Corrosion may not be mediated by simply killing the planktonic microorganisms. Biofilm removal through chemical and/or mechanical cleaning is usually necessary. Corrosion can be substantially mediated by inhibiting microorganism metabolism with proper choice of a biocide program.
Algae uses energy from the sun to convert bicarbonate or carbon dioxide into biomass. Algal mass can block piping, distribution holes, and nozzles.
Macro higher forms are bioincrustations colonized by large organisms. Macrofouling is common to once-through cooling systems due to buildups or infestations of Asiatic clams, zebra mussels or barnacles, bryozoans, and/or hydroids in marine environments at water intakes.
Eliminating sunlight from wetted surfaces such as distribution troughs, cooling media, and sumps significantly reduces algal growth. A distribution deck cover, which drastically reduces the sunlight reaching the algae in the water, is one of the most cost-effective control devices for a cooling tower.
Eliminating dead legs and low-flow areas in the piping and the cooling loop reduces biological growth in those areas. Careful selection of materials of construction can remove nutrient sources and environmental niches for growth and helps mitigate corrosion. Maintaining a high-quality disinfected makeup water supply with low turbidity and bacterial counts reduces biological growth. Equipment should be designed with adequate access for inspection, sampling, and manual cleaning.
Mechanical aids include submicron filter media, fine strainers, scrapers/brushes, and flow and temperature control. Nonchemical treatment approaches include biocidal paint, ultraviolet light, sonication with ultrasound, and modification of contact surface material.
Usually, effective control of slime and algae requires a combination of mechanical and chemical treatments. For example, when a system already contains a considerable accumulation of slime, a preliminary mechanical cleaning makes the subsequent application of a biocidal chemical more effective in killing the growth and more effective in preventing further growth. A build-up of scale deposits, corrosion products, and sediment in a cooling system also reduces the effectiveness of chemical biocides. Routine disinfection of cooling towers, including the use of high-level chlorination and a biodispersant, helps control Legionella as well as other microorganisms. Sidestream filtration and monitoring devices such as corrosion coupons, test spools, and biofilm sensors can enhance monitoring of biofilm growth. Alternating two different types of biocides can overcome resistance developed by bacteria against a single biocide. The two different types should include two different kill mechanisms.
More cooling-water treatment programs fail because of lack of microbiological monitoring and control than from any other treatment problem. Scale, corrosion, and fouling are often symptoms of poor microbiological control. Corrosion often occurs under bacterial slime layers. Inorganic foulants are trapped in slime layers, compounding problems. The effects of uncontrolled microbiological activity and fouling may negate the effectiveness of even the best programs for scale prevention and corrosion inhibition. Appropriate biocides must be selected to handle the most prevalent problems first, perhaps in conjunction with dispersants to penetrate and remove deposits. Effective microbiological control is an absolute necessity for an open cooling-water program to be successful.
An effective microbicide (biocide) program has five steps:
-
Identify the types and concentrations of microorganisms present in the system.
-
Select proper biocides based on system design, discharge restrictions, and types of microorganisms.
-
Implement proper application, dosage, contact time, and control of the selected biocides.
-
Perform seasonal disinfection cleanings.
-
Understand system operation and piping layout to determine appropriate water sampling points to indicate worst system water conditions.
Microbicides. Chemical biocides used to control biological growth in cooling systems fall into two broad categories: oxidizing and nonoxidizing. There are numerous options commercially available. Some address a broad spectrum of organisms, whereas others are used to target specific types of organisms such as algae, SRBs, or fungi. Selection of the biocides should always be left to water treatment professionals.
Effective biocide treatment is usually a combination of an oxidizing biocide with a nonoxidizing biocide. The oxidizer may be fed continuously or intermittently. Nonoxidizing biocide may be introduced with either oxidizing biocide strategy. Oxidizing biocides provide quick-kill results and are best used to control biofilm; nonoxidizers are relatively slow acting and best used to suppress MIC activity. A biodispersant (surfactant) is often also incorporated to enhance biocide performance.
Oxidizing Biocides. These substances (chlorine, bromine, ozone, iodine, chlorine dioxide, and halogen-releasing compounds such as bromochlorodimethylhydantoin [BCDMH or BCD]) are among the most effective biocide chemicals used in water treatment. However, they are not always effective or appropriate for use in cooling-water systems with high organic loading, high temperatures, and/or systems with corrosion or contaminant (compatibility) issues. Chlorine dioxide is probably the one oxidizing biocide least affected by high chemical oxygen demand (COD) and total organic carbon (TOC). In air washers, the odor may become offensive to building/facility occupants, or the exit air (to the building/facility) may be too corrosive for the environment. In wooden cooling towers, high levels of oxidizing biocides can cause delignification. Overdosing of oxidizing biocides may cause corrosion issues with metallic components in any system. Accurate feed and control of oxidizing biocides for the most effective, efficient, and safe application requires using appropriate feed and control equipment. In many systems, the most effective use of oxidizing biocides is to maintain a constant, low-level residual in the system. However, if halogen-based oxidizing biocides are fed intermittently (slug dosed), a pH below 8 is most advantageous, because of the pH-dependent dissociation curve where the halogen (particularly chlorine) is more prevalent in the more biocidal active (hypohalous acid) form. The residual oxidizing biocide concentration should be tested on a routine basis. Most halogenation programs can benefit from using dispersants or surfactants to penetrate and break up microbial masses and biofilm.
Chlorine has been the oxidizing biocide of choice for many years, either as chlorine gas, or in liquid form as sodium hypochlorite. Other forms of chlorine are available, such as powders, pellets, or calcium hypochlorite sticks; chlorine-releasing compounds (e.g., chloramines, chloroisocyanurates). It can also be produced electrolytically with brine on site. Use of chlorine gas is declining because of health and safety concerns involved in handling it and because of environmental pressures concerning the formation of EPA-regulated halogenated disinfection by-products. In hot-water systems, including potable hot-water systems, chlorine loses efficacy up to 70% at temperatures of 60 to 71°C.
Bromine is usually produced through reactions of an oxidizer such as sodium hypochlorite with sodium bromide on site, or by release from solids of chlorobromohydantoin compounds. Bromine has certain advantages over chlorine: it is less volatile, and bromamines break down more rapidly than chloramines in the environment. Also, when slug feeding biocide in high-pH systems, hypobromite ions may have an advantage because their biocidal power is better than that of hypochlorite ions. This effect is less important when biocides are fed continuously at low dosage. Like chlorine, bromine can affect the environment with formation of EPA-regulated halogenated disinfection by-products.
Ozone is a gaseous form of oxygen consisting of three oxygen atoms (O3). As a biocide, it has several advantages compared to chlorine: it does not produce halogenated disinfection by-products, it breaks down to nontoxic compounds rapidly in the environment, it is more potent than chlorine in decomposing organics destructing biofilms, and it requires significantly less chemical handling. The disadvantages of ozone are its short half-life, instability for storage (requiring on-site generation), and stringent EPA regulations on ozone reaction by-products. Use of ozone-generating equipment in an enclosed space requires safety protocols to protect operators from toxic gas.
Water conditions should be reviewed to determine the need for scale and corrosion inhibitors and then, as with all oxidizing biocides, inhibitor chemicals should be carefully selected to ensure compatibility. To maximize the biocidal performance of ozone, the injection equipment should be designed to provide adequate contact time of the ozone with the circulating water. In larger systems, ensure that the ozone is not depleted before ozonated water has circulated through the entire system.
Iodine is provided in pelletized form, often from a rechargeable cartridge. Iodine is a relatively expensive chemical for use on cooling towers and is probably only suitable for use on smaller systems.
Chlorine dioxide gas is effective in low concentrations (0.2 to 0.8 mg/L residual). It must be generated on site. Unlike ozone, it is not affected by pH, and has a longer half-life and therefore a higher penetrating power because of lower oxidizing potential. It is usually generated with sodium chlorite precursor by either an electrolytic generator or reactions with acids. Its drawbacks are instability in storage, costly generating equipment, and precursors and acid salt in the end-product solution as well as safety issues with precursor chemicals.
Hydrogen peroxide (H2O2) is a liquid that is usually available in concentrations of 35% or less, by mass, in water. Hydrogen peroxide is considered one of the most environmentally friendly oxidizing biocides, because it degrades to water. However, instability and the potential danger in handling concentrated hydrogen peroxide suppress its widespread use in high concentrations. It is usually used with a stabilizer to form peracetic acid.
Nonoxidizing Biocides. These biocides destroy organisms either by poisoning the organism, blocking its ability to uptake energy, or disrupting its protective coating (cellular membranes) and exposing the organism to a hostile environment. Most nonoxidizers are also known as biostats, which means they inhibit growth of microorganisms.
When selecting a nonoxidizing biocide, many factors must be considered for its effective and efficient use, including system pH and relevant water chemistry, chemical compatibility with other treatment products and system contaminants, and the system turnover rate, or holding time index (HTI), for adequate microbial contact time. Common nonoxidizing biocides include the following:
-
Quaternary ammonium compounds
-
Polyquats
-
Methylene bis(thiocyanate) (MBT)
-
Isothiazolones
-
Tetrahydro-3,5-dimethyl-2H-1,3,5-thiadiazine-2-thione (Thione)
-
Tributyl tetradecyl phosphonium chloride (TTPC)
-
Bis(tributyltin) oxide (TBTO)
-
Carbamates/Dithiocarbamates
-
2-(Decylthio)ethanamine (DTEA)
-
Glutaraldehyde
-
Dodecylguanidine (Guanides)
-
Tetrakish(hydroxymethyl)phosphonium sulfate (THPS, TKHPS)
-
2-(tert-butylamino)-4-chloro-6-(ethylamino)-s-triazine (TBZ,Tertbuthylazine)
-
2-2-Dibromo-3-nitrilopropionamide (DBNPA)
-
2-Bromo-4-hydroxyacetophenone (BHAP)
-
2-Bromo-2-nitropropane-1,3-diol (Bronopol)
-
Bromo-nitrostyrene (BNS)
-
Proprietary blends
-
Aldehyde release treatments
-
Organosulfur compounds
How nonoxidizing biocides are fed is important. Sometimes, the continuous feeding of low dosages is neither effective nor economical. Slug feeding large concentrations to achieve a toxic level of the chemical in the water long enough to kill the organisms present can show better results. Water blowdown rate and biocide hydrolysis (chemical degradation) rate affect the required dosage. The hydrolysis rate of the biocide is affected by the type of biocide, along with the temperature and pH of the system water. Dosage rates are proportional to system volume; dosage concentrations should be sufficient to ensure that the contact time of the biocide is long enough to obtain a high kill rate of microorganisms before the minimum inhibitory concentration of the biocide is reached. The period between nonoxidizing biocide additions should be based on the system half-life, with sequential additions timed to prevent regrowth of bacteria in the water. When two nonoxidizing biocides are used, it is important to select the two biocides based on two different kill modes to overcome resistance developed by microbes.
Other Biocides. Ultraviolet (UV) irradiation deactivates microorganisms by cleaving DNA and nucleic acid molecules as the water passes around a quartz tube containing the UV lamp. The UVC spectrum covers the 200 to 280 nm wavelength, with most sources producing 254 nm light. The intensity of the light, thorough contact with the water, and adequate contact time are critical in obtaining a satisfactory kill of microorganisms. Suspended solids in the water or deposits on the quartz tubes significantly reduce the effectiveness of this treatment method. Therefore, a filter is often installed upstream of UV lamps to minimize these problems. Because UV light leaves no residual biocide in the water, sessile organisms and organisms that do not pass the light source are not affected by UV treatment. UV irradiation may be effective in humidifiers and air washers where the application of biocidal chemicals is unacceptable and where 100% of the recirculating water passes the lamp. It is less effective where all microorganisms cannot be exposed to the treatment, such as in cooling towers. Ultraviolet lamps require replacement after approximately every 9000 to 10,000 h of operation. The glass sleeves slowly accumulate deposits and become opaque to UV light, despite the use of wipers to keep the surface clean. UV lamp electrodes contain mercury, which requires special disposal for environmental protection. UV light can also be used to decompose chemical oxidants either to neutralize the residual oxidant or to promote advanced oxidation processes.
Copper (Cu) and silver (Ag) ions can effectively control microbial populations in water systems when the ionization systems that produce them are properly maintained, operated, and applied. Ions are released into the water via electrochemical means to generate 0.4 to 0.8 mg/L of copper and/or 40 to 80 μg/L of silver. The ions assist in the control of bacterial populations by interfering with electron transfer and denaturing protein by reacting with sulfydryl, amino, and carboxylate groups. Copper, in particular, effectively controls algae. Cu and Ag treatment is not suitable for hard and alkaline waters. Prolonged treatment (over 3 years) can develop resistant strains.
Handling Biocides. All biocides must be handled with care to ensure personal safety. In the United States, cooling-water biocides are approved and regulated through the EPA and, by law, must be handled in accordance with labeled instructions. Maintenance staff handling the biocides must read the safety data sheets (SDS) and be provided with all appropriate safety equipment to handle each substance. An automatic feed system is preferred to minimize and eliminate handling of biocides by maintenance personnel. Several U.S. states (e.g., New York, New Jersey, Pennsylvania, Connecticut, Ohio, Rhode Island, Vermont, Indiana) require certified personnel to handle biocides.
Legionella and Legionnaires’ Disease
Legionellosis is any disease caused by Legionella bacteria. Legionnaires’ disease, a form of Legionellosis, is a potentially fatal, pneumonia-like illness primarily caused by Legionella pneumophila serogroup 1 (Lp 1), one of the more than fifty known species of Legionella.
Legionellae are common warm-water, aerobic, gram-negative microorganisms that are mostly found in surface waters (lakes, ponds, rivers, streams) but can also be found in groundwater sources, including some soils. They tend to grow in biofilm or slime on the surfaces of lakes, rivers, and streams. Legionellae adapt to conditions in water distribution systems, thereby sometimes escaping municipal water plant disinfection (chlorination). They can, therefore, be found in domestic (potable) water plumbing and associated building water systems such as cooling towers, spas, water fountains, and other water-use systems. Within these systems, Legionella can find favorable conditions for growth and amplification, and pose a risk for human disease.
The mere presence of Legionella does not necessarily result in disease. Several conditions and factors must occur: primarily, there must be enough and/or virulent forms of the bacteria made transmittable and then transmitted to a susceptible host. Transmission occurs when a host inhales tiny water droplets (mists or vapor aerosols) containing Legionella from a water-aerosolizing source. Aspiration of water can also occur during normal drinking and swallowing due to choking or gag reflex. Inhalation can bring infectious Legionella to the deep, distal parts (alveoli) of the lungs, where they take over and promote the pneumonia of Legionnaires’ disease. The dose of Legionella pneumophila (or other species of Legionella) required to infect humans is not known, and is most probably influenced by host susceptibility.
Legionellae grow well and amplify in warm water environments and systems that provide favorable conditions for bacterial growth and the formation of biofilm. The optimum temperature range for growth is 32 to 41°C. The subsequent use of water from such systems harboring Legionella, through faucets, shower sprays, humidifying, aerosolizing (misting) devices, or other spray or drift mechanisms of the system may transmit the bacteria to susceptible hosts.
Legionella pneumophila was first identified in 1977, following an outbreak of disease associated with a Philadelphia host hotel for an American Legion bicentennial convention in 1976. Since then, surveillance systems and research studies have been established around the world. In recent years, with improved capabilities and changes in clinical methods of diagnosis, there has been an upsurge in reported cases in many countries. Environmental studies continue to provide information and identify novel sources of infection, leading to regular revisions of guidelines and regulations. The number of cases reported to the CDC has been on the rise since 2000. Health departments reported nearly 10,000 cases of Legionnaires’ disease in the United States in 2018. However, because Legionnaires’ disease is likely underdiagnosed, this number may underestimate the true incidence. A recent study estimated that the true number of Legionnaires’ disease cases ma be 1.8 to 2.7 times higher than what is reported. More illness is usually found in the summer and early fall, but it can happen any time of year. About 1 in 10 people who get sick from Legionnaires’ disease will die.
Outbreaks of Legionnaires’ disease receive media attention. However, this disease more often occurs as single, isolated cases not associated with any recognized outbreak. When outbreaks occur, they are usually in the summer and early autumn, though cases may occur at any time of year.
Water treatment microbial control programs should also include a risk assessment for Legionella control and disease prevention. This includes the effectiveness of treatment products and the program to control Legionella and the conditions favorable for its growth and amplification, including the accumulation of biofilm (slime/biomass), the presence of amoebae and other protozoans that harbor it, as well as the potential of the water system to produce aerosols and provide routes of aerosol transmission to susceptible human populations.
See ASHRAE Standard 188-2021 and ASHRAE Guideline 12-2020 for further information.
2.4 NONCHEMICAL AND PHYSICAL WATER TREATMENT METHODS
Nonchemical water treatment has been used for boiler water, cooling water, potable water, and other process applications for decades. There are multiple classifications of such treatment methods and equipment systems. Adherence to manufacturers’ recommendations and the proper application of these technologies is critical to achieving successful results. As with traditional methods of water treatment, the ability to achieve successful results should be adequately evaluated for the water treatment system as well as regularly monitored for effective control of scale, corrosion, and biological contamination. Water treatment technologies, published papers, and case histories should be evaluated considering water supply chemistry, operating environment, duty, and industry standard performance metrics.
Several nonchemical and physical water treatment equipment technologies are classified in the following paragraphs, along with brief summaries of their basic claims and theoretical mechanisms of action.
Magnetic, or fixed-field magnetic, systems are designed to cause scale-forming minerals to precipitate on suspended solids as opposed to heat exchanger surfaces. This mechanism produces nonadherent particles, often classified as the aragonite form of calcium carbonate versus the hard, adherent calcite. The precipitated particles can then be removed by blowdown, mechanical means, or physical flushing.
Electromagnetic systems induce either a constant or variable magnetic flux density (or both), thereby inducing a localized, variable electric field in the bulk water. Pulsed-power and electrodynamic field systems generate a combination of variable magnetic flux density with a variable electric field at frequencies greater than the incoming line signal. The induced electric fields alter the surface charge on suspended solids and particulates, and force precipitation on these surfaces in the bulk water.
Cavitation systems can cause formation and sudden collapse of low-pressure bubbles in a water stream by means of a mechanical force. The collapse of the bubbles imparts a shock wave and resultant heat locally within the water flow. The energy created during the implosion of bubbles promotes precipitation of minerals in the water stream.
Ionization rods create a static electric field that disperses scale-producing foulants, thereby inhibiting precipitation of minerals on equipment surfaces. The dispersion created by the device's electric field also inhibits biological growth.
Electrolysis systems pass an electric current between two electrodes. Precipitation of minerals occurs at the cathode. Biological growth is inhibited by formation of chlorine gas at the anode; the gas combines with water to form hypochlorite.
Ultrasonic systems impart ultrasonic acoustic energy to a stream of water. The sound wave produced by ultrasonic devices can cause mechanical damage to bacteria cell walls. Like cavitation devices, ultrasonic energy can also produce low-pressure bubbles, which can collapse and damage bacterial cell walls.
Ultraviolet light systems irradiate a water stream with ultraviolet light. Exposing microorganisms to ultraviolet light inhibits their biological growth. The ability to effectively and efficiently control microbial populations throughout a cooling-water system with a point-of-use ultraviolet light system must be evaluated for any given system.
Ozone systems inject ozone created by coronal plasma, by ultraviolet lamps, or by chemical reaction, into the bulk water. When contact is made with microorganisms, ozone can be a very effective disinfectant for their control. However, it is difficult to maintain an effective residual of ozone throughout a cooling-water system because of its high reactivity and fast dissipation. Ozone is very volatile and can be lost from the system as the water passes through the cooling tower fill. Successful application of ozone for biological control requires that sufficient ozone-generating capacity be provided to sustain a level of ozone residual that will control microbial contamination throughout the cooling-water system.
ASHRAE research projects RP-765 (Nasrazadani and Chao 1996) and RP-747 (Gan et al. 1996) found ozone only marginally effective in scale and corrosion inhibition, respectively. Ozone has been shown to have a very limited and unpredictable effect on calcium carbonate scale, and a limited effect to inhibit corrosion of most metals. It provides some reduction of mild steel corrosion, but increases the corrosion rates of copper and copper alloys. It is also known to attack galvanized steel, and increasing the level of ozone in water increases the corrosiveness of the water.
ASHRAE research project RP-1155 (Cho 2002) studied physical water treatment with respect to scale prevention and/or mitigation. For the study, a physical water treatment (PWT) device was defined as a nonchemical method of water treatment for scale prevention or mitigation. Bulk precipitation on colloidal surfaces was proposed as the mechanism of scale prevention. Three different PWT devices (permanent magnets, a solenoid coil device, and a high-voltage electrode) were tested under laboratory conditions. Fouling resistance data obtained in a heat transfer test section supported the benefit of all three devices when configured in optimum conditions in the laboratory-scale test system.
ASHRAE research project RP-1361 (Vidic et al. 2010) studied physical water treatment and microbial control. In this study, a PWT device was defined as a nonchemical method of water treatment for microbial control. Five different PWT devices (magnetic, pulsed electric field, electrostatic, ultrasonic, and hydrodynamic cavitation) were tested in a pilot-scale cooling tower. No statistically significant difference in planktonic or sessile microbial concentrations was observed in the (test) pilot-scale cooling tower for any of the devices, as compared to an untreated control tower.
Copies of ASHRAE research project final reports can be obtained from technologyportal.ashrae.org, and are free to ASHRAE members.